AS far as painting above the water line,sand with 100 grit sand paper and fill all inperfections, apply Awlgrip 545 primer, sand with 220 grit for light colors 300 grit for dark, now spray or brush awlgrip, spray 3-4 coats, brush 2 coats. Mix for spaying 50/50,half paint half catalist, mix for brushing 50/25 or two parts paint one part catalist, reduce up to 25% for spaying and 10% for brushing. Make sure you wait 30 to 40 minutes bettween coats anless you add X-98 then as soon as drie to the touch spray another coat. Other things you may want Crater-X fish eye remover and Awl-400 wipedown solution get a US paints Awlgrip manuel and study it Awlgrip is expensive do it right the first time.